What cut quality before forming means at 152 → 114 mm
If you are holding a drawing with 152 → 114 mm on it and Chromoly 4130 (30KhGSA) in the material box, the cut quality before forming call is a cut held to ±0.8 mm with burr under 0.20 mm, because a burr that survives forming becomes a crack initiation site at the tip. We build that number from the reduction ratio, the wall and the yield strength, in that order, because those three move it and nothing else does.
The die meets the tube edge before anything else. A square, burr-free cut is the cheapest quality improvement in the whole line, and a bad one mimics every die fault there is.
The two numbers that matter
Squareness within 0.5 mm across the diameter, and burr under 0.2 mm on the inside. A slanted face makes the die contact a line rather than a ring: the high side takes all the load first, the cone comes out oval, and the operator blames the die. Springback adds 0.29 mm to the tip diameter, so the die is cut that much under nominal.
An internal burr is worse because it is invisible. It gets rolled into the cone wall, leaves a fold line, and on a fatigue part becomes the crack origin. You cannot inspect it from outside after forming. 3,991 pieces per die set is the working number here; below 1,996 pieces a year the tooling never pays back.
What to change, and in what order
Clamp pressure first — a loose clamp on a cold saw produces a slanted cut with a perfect blade. Then blade condition, then feed rate. On a CNC tube cutter, the chamfer head removes the burr in the same cycle and is usually cheaper than a separate deburr station. The 2.2 per cent scrap allowance is not padding — it is the pass count and the material talking.
Abrasive saws cut fast and leave a heat-affected edge and a heavy burr. They are acceptable for structural parts and unacceptable for anything that will be tapered and then loaded. The mill certificate matters more than the grade name: spread inside the standard moves the force by about 75 kN.
The numbers for this combination
| Tube outside diameter | 152 mm |
| Small-end diameter | 114 mm |
| Wall thickness | 6.0 mm |
| Cone length | 250 mm |
| Reduction on diameter | 25.0 per cent |
| Half angle / included angle | 4.35° / 8.7° |
| Yield strength used | 435 MPa |
| Forming force, single bite | 1,250 kN |
| Forming force, per bite at 2 passes | 693 kN |
| Passes | 2 passes |
| Process | cold forming |
| Cycle time | 17.9 s |
| Output per 8 h shift | 1,319 pieces |
| Tip wall after forming | 6.93 mm (+15 per cent) |
| Springback on tip diameter | 0.29 mm |
| Ovality at the tip | 0.8 per cent |
| Blank length | 427 mm |
| Blank weight | 9.22 kg |
| Machine class | L-160×600 CNC |
Computed for this combination. Confirm the force and the tip wall on a sample before the die is cut.
Cycle time is measured from tube-in to tube-out with the operator loading by hand. Automated loading cuts the handling element, not the forming element, so the saving is smaller than the brochure implies at this size — about a fifth of 17.9 s.
Where a number depends on the heat of steel rather than on the geometry, it is flagged. Those are the figures to re-measure on the first batch instead of copying from this page.
How Chromoly 4130 (30KhGSA) behaves at 25.0 per cent reduction
The fork-shaft standard. Higher yield means higher tonnage and stronger springback, and it work-hardens quickly, so a second pass on an already formed cone is not an option.
Yield strength drives the force linearly, so the jump from 235 MPa to 435 MPa is a 85 per cent heavier bite at the same geometry. Ductility drives everything else: pass count, edge condition, whether the tip cracks before the die is dialled in.
Normalise or anneal before forming if the tube arrives cold-drawn; stress relief after forming is normal practice.
Extra-large section: 152 → 114 mm
Extra-large cones are almost always hot formed or formed in two stages. The wall is thick enough that cold flow becomes unpredictable and the die sees loads that shorten its life fast.
Dies for this size are 90 kg and up: light enough to change by hand on the small end, heavy enough that a two-person lift is the safe rule at the top of the range.
If this size is a one-off rather than a family, consider buying the die and subcontracting the run. At 3,991 pieces of die life, a single order under 1,996 pieces rarely justifies the tooling on its own.
Cost per 1,000 pieces
| Metal in the blank | 9.22 kg, 14.759 USD |
| Machine time | 17.9 s, 0.273 USD |
| Die cost, one set | 7,540 USD |
| Die life | 3,991 pieces |
| Scrap allowance | 2.2 per cent |
| Cost per piece | 17.30 USD |
| Cost per 1,000 | 17,303 USD |
Metal is 85 per cent of the piece cost at this combination. That ratio is the reason a cheaper machine rarely changes the verdict: shaving ten per cent off the machine rate moves 17.30 USD by 0.027 USD, while shaving ten per cent off the blank moves it by more.
What to put on the drawing
Add the as-formed wall at the tip as a reference dimension with a minimum. It is the dimension that decides whether the mating bore cleans up, and it is the one most often left off.
Put the two diameters, the cone length and the wall on the drawing as basic dimensions, then tolerance the cone angle rather than the tip diameter. A tip diameter tolerance of ±0.2 mm is a different requirement at 152 mm than it is at 32 mm, and the die grinder needs to know which one you mean.
If you cannot state the cone length because the part is defined by a mating component, send the mating component instead. We will derive the cone and tell you what the resulting angle is before quoting.
Frequently asked questions
Does cut quality matter on thick wall?
Less for cracking, more for squareness. A thick wall forgives the burr and punishes the angle.
Can I inspect burr without pulling parts?
A mirror and a torch at the machine, ten parts an hour. Cheaper than the scrap it prevents.
Does the cut affect cycle time?
Only through rework. A part that needs deburring adds 5–15 seconds that never appear in the cycle-time quote.
Does the heat treatment number change with wall thickness?
Yes — soak time scales with section, not with the part. 620 °C is right for this grade, but a 6.0 mm wall needs the 1 h per 25 mm of section at temperature, not the twenty-minute cycle that works on thin sheet.
What tube tolerance should I buy?
±0.15 mm on outside diameter and ±10 per cent on wall for this geometry. Tighter than that costs money at the mill and buys you nothing the die cannot absorb; looser than that and the 0.8 per cent ovality figure stops holding.
Talk to an engineer on WhatsApp
Send your tube drawing, material and target output. We will reply with a machine configuration, a measured sample plan and a factory quotation. WhatsApp +86 183 0020 2909 or email info@jixin.online.
Chat on WhatsApp