What cut quality before forming means at 76 → 48 mm
Short version for Chromoly 4130 (30KhGSA) at 76 → 48 mm: a cut held to ±0.5 mm with burr under 0.15 mm, because a burr that survives forming becomes a crack initiation site at the tip. It is worth knowing why before you accept it, because the same three inputs that produce this answer will produce a different one the moment the wall or the grade changes.
The die meets the tube edge before anything else. A square, burr-free cut is the cheapest quality improvement in the whole line, and a bad one mimics every die fault there is.
The two numbers that matter
Squareness within 0.5 mm across the diameter, and burr under 0.2 mm on the inside. A slanted face makes the die contact a line rather than a ring: the high side takes all the load first, the cone comes out oval, and the operator blames the die. The mill certificate matters more than the grade name: spread inside the standard moves the force by about 26 kN.
An internal burr is worse because it is invisible. It gets rolled into the cone wall, leaves a fold line, and on a fatigue part becomes the crack origin. You cannot inspect it from outside after forming. At this size the die sees 243 kN per bite, which is why the L-120×400 F is the natural home for the job.
What to change, and in what order
Clamp pressure first — a loose clamp on a cold saw produces a slanted cut with a perfect blade. Then blade condition, then feed rate. On a CNC tube cutter, the chamfer head removes the burr in the same cycle and is usually cheaper than a separate deburr station. Running 2 passes puts the cycle at 13.6 s and the shift output near 1,736 pieces.
Abrasive saws cut fast and leave a heat-affected edge and a heavy burr. They are acceptable for structural parts and unacceptable for anything that will be tapered and then loaded. The tip wall finishes at 4.40 mm, 26 per cent heavier than the 3.5 mm you started with — plan the mating bore around that and not around the blank.
The numbers for this combination
| Tube outside diameter | 76 mm |
| Small-end diameter | 48 mm |
| Wall thickness | 3.5 mm |
| Cone length | 120 mm |
| Reduction on diameter | 36.8 per cent |
| Half angle / included angle | 6.65° / 13.3° |
| Yield strength used | 435 MPa |
| Forming force, single bite | 438 kN |
| Forming force, per bite at 2 passes | 243 kN |
| Passes | 2 passes |
| Process | cold forming |
| Cycle time | 13.6 s |
| Output per 8 h shift | 1,736 pieces |
| Tip wall after forming | 4.40 mm (+26 per cent) |
| Springback on tip diameter | 0.13 mm |
| Ovality at the tip | 1.2 per cent |
| Blank length | 214 mm |
| Blank weight | 1.34 kg |
| Machine class | L-120×400 F |
Computed for this combination. Confirm the force and the tip wall on a sample before the die is cut.
The force figure is the one people misread. 438 kN is what a single bite taking the whole 36.8 per cent reduction would need; the press in the schedule only sees 243 kN because the reduction is split. Quoting the first number for a multi-pass job is how machines get bought one size too large.
Read the table before the prose if you are in a hurry. The table is the part you can defend in a meeting; the prose explains which entries are sensitive to the material certificate and which are not.
How Chromoly 4130 (30KhGSA) behaves at 36.8 per cent reduction
The fork-shaft standard. Higher yield means higher tonnage and stronger springback, and it work-hardens quickly, so a second pass on an already formed cone is not an option.
Chromoly 4130 (30KhGSA) at this reduction behaves like a workable material, and the schedule above is written for that. Push the reduction per pass and the failure mode is a roughened cone that needs polishing, not a slow drift out of tolerance.
Typical use for this grade is e-bike and motorcycle fork shafts, suspension tubes, motorsport parts. If your part sits outside that list, the numbers still apply but the corrosion and fatigue assumptions behind them do not.
Large section: 76 → 48 mm
At 76 mm the force starts to matter: the same wall needs roughly twice the tonnage of a 60 mm part, and the guide bushing has to control a heavier tube.
At 76 mm the guide bushing matters as much as the die. A 76 mm tube has enough length to lever against the die entry if the bushing clearance is loose, and the symptom is ovality at the tip that looks like a die problem and is not.
Floor space and power follow the class, not the part: a L-120×400 F needs the footprint in its own datasheet whether you run 76 mm or something smaller in it.
Cost per 1,000 pieces
| Metal in the blank | 1.34 kg, 2.143 USD |
| Machine time | 13.6 s, 0.113 USD |
| Die cost, one set | 2,860 USD |
| Die life | 14,254 pieces |
| Scrap allowance | 2.2 per cent |
| Cost per piece | 2.51 USD |
| Cost per 1,000 | 2,512 USD |
Scrap is priced into 2.51 USD at 2.2 per cent. If your first article runs clean, the real cost is lower than this; if it does not, this number was optimistic and the difference shows up as a month of rework.
What to put on the drawing
Say what happens after forming: machined, welded, coated, or used as formed. The allowance, the stress relief and the surface spec all follow from that one line.
Add the as-formed wall at the tip as a reference dimension with a minimum. It is the dimension that decides whether the mating bore cleans up, and it is the one most often left off.
Send the drawing as a PDF with the dimensions readable at 100 per cent. Half the quotation delays we see come from a photo of a printout, not from a hard part.
Frequently asked questions
Does cut quality matter on thick wall?
Less for cracking, more for squareness. A thick wall forgives the burr and punishes the angle.
Can I inspect burr without pulling parts?
A mirror and a torch at the machine, ten parts an hour. Cheaper than the scrap it prevents.
Does the cut affect cycle time?
Only through rework. A part that needs deburring adds 5–15 seconds that never appear in the cycle-time quote.
Is 4130 chromoly suitable for a part that will be welded after forming?
It welds, but the formed tip is work-hardened and the weld pool will dilute that. For a structural weld, stress relieve at 620 °C first, or move the weld away from the cone.
Would a smaller machine do this job?
Not at 243 kN per bite with a 76 mm tube to guide. The L-120×400 F is the smallest class that holds the die squarely at this diameter; a lighter frame deflects and the ovality shows up before the force limit does.
Talk to an engineer on WhatsApp
Send your tube drawing, material and target output. We will reply with a machine configuration, a measured sample plan and a factory quotation. WhatsApp +86 183 0020 2909 or email info@jixin.online.
Chat on WhatsApp