What surface finish for coating means at 60 → 38 mm
If you are holding a drawing with 60 → 38 mm on it and Chromoly 4140 (42CrMo / 40KhM) in the material box, the surface finish for coating call is Ra 1.2 µm on the cone flank straight out of the die, with no secondary polishing step in the routing. We build that number from the reduction ratio, the wall and the yield strength, in that order, because those three move it and nothing else does.
A formed cone has a directional die texture. Under 60–80 microns of powder it telegraphs through, and at the tip edge the film pulls back to half thickness.
What the coater needs from the die
A fine, even texture rather than a polished mirror. Polishing looks better before coating and adheres worse after it, because there is no mechanical key. A light blast on the cone followed by phosphate is the combination that survives a salt spray test. The tip wall finishes at 3.14 mm, 26 per cent heavier than the 2.5 mm you started with — plan the mating bore around that and not around the blank.
The tip edge needs a radius of about 0.5 mm. A sharp edge holds 15 microns where a radius holds 40, and the edge is where rust starts on every outdoor part. Budget 1.34 USD per piece at this combination, of which 79 per cent is metal.
The defects that only appear after curing
Outgassing pinholes come from air or moisture trapped in a lap or a porous weld, expanding at curing temperature. The fix is upstream: find the lap and stop making it. Springback adds 0.17 mm to the tip diameter, so the die is cut that much under nominal.
Edge pull-back is a coverage problem, not an adhesion problem, and adding a second coat does not fix it because the second coat pulls back too. 15,698 pieces per die set is the working number here; below 7,849 pieces a year the tooling never pays back.
The numbers for this combination
| Tube outside diameter | 60 mm |
| Small-end diameter | 38 mm |
| Wall thickness | 2.5 mm |
| Cone length | 95 mm |
| Reduction on diameter | 36.7 per cent |
| Half angle / included angle | 6.60° / 13.2° |
| Yield strength used | 655 MPa |
| Forming force, single bite | 371 kN |
| Forming force, per bite at 3 passes | 146 kN |
| Passes | 3 passes |
| Process | cold forming |
| Cycle time | 15.5 s |
| Output per 8 h shift | 1,523 pieces |
| Tip wall after forming | 3.14 mm (+26 per cent) |
| Springback on tip diameter | 0.17 mm |
| Ovality at the tip | 1.6 per cent |
| Blank length | 171 mm |
| Blank weight | 0.606 kg |
| Machine class | L-120×400 F |
Computed for this combination. Confirm the force and the tip wall on a sample before the die is cut.
The blank length assumes you grip 66 mm of straight tube in the collet and trim 10 mm after forming. If your chuck is longer, add it to 171 mm — the cone itself does not change, only the material you pay for.
Read the table before the prose if you are in a hurry. The table is the part you can defend in a meeting; the prose explains which entries are sensitive to the material certificate and which are not.
How Chromoly 4140 (42CrMo / 40KhM) behaves at 36.7 per cent reduction
Supplied usually as quenched and tempered, which is exactly the wrong condition for cold forming. Either form it in the annealed state and harden afterwards, or expect a very narrow process window.
Yield strength drives the force linearly, so the jump from 235 MPa to 655 MPa is a 179 per cent heavier bite at the same geometry. Ductility drives everything else: pass count, edge condition, whether the tip cracks before the die is dialled in.
At 36.7 per cent reduction the work-hardening from forming is worth roughly 144 MPa of extra yield at the tip. If your next operation is machining, that is helpful; if it is another forming pass, budget for it.
Medium section: 60 → 38 mm
The 60 to 38 pair is the workhorse of the trade: fork blanks, furniture legs, pole sections. Tonnage is moderate and almost every machine size can do it, so the decision usually turns on cycle time and die life.
Dies for this size are 40 to 60 kg: light enough to change by hand on the small end, heavy enough that a two-person lift is the safe rule at the top of the range.
Machine class for 60 mm is the L-120×400 F. Going one class up buys stiffness you will not use at this diameter and costs floor space you will miss.
Cost per 1,000 pieces
| Metal in the blank | 0.606 kg, 1.061 USD |
| Machine time | 15.5 s, 0.103 USD |
| Die cost, one set | 2,030 USD |
| Die life | 15,698 pieces |
| Scrap allowance | 3.7 per cent |
| Cost per piece | 1.34 USD |
| Cost per 1,000 | 1,343 USD |
The 1.34 USD figure excludes finishing, coating and packing. It is the formed part at the machine, which is the only number that lets you compare two processes fairly.
What to put on the drawing
Say what happens after forming: machined, welded, coated, or used as formed. The allowance, the stress relief and the surface spec all follow from that one line.
Add the as-formed wall at the tip as a reference dimension with a minimum. It is the dimension that decides whether the mating bore cleans up, and it is the one most often left off.
If you cannot state the cone length because the part is defined by a mating component, send the mating component instead. We will derive the cone and tell you what the resulting angle is before quoting.
Frequently asked questions
Can a formed cone be galvanized?
Yes, with drain holes and a wall thick enough not to distort at 450 °C. Thin-wall cones warp.
Does the die texture affect coating cost?
Indirectly: a rough cone needs more pretreatment and sometimes a primer, which is a per-part cost forever.
What surface roughness should I specify?
Ra 1.6–3.2 on the cone is a practical range for powder. Finer is not better without a blast.
Is 4140 chromoly suitable for a part that will be welded after forming?
It welds, but the formed tip is work-hardened and the weld pool will dilute that. For a structural weld, stress relieve at 620 °C first, or move the weld away from the cone.
Would a smaller machine do this job?
Not at 146 kN per bite with a 60 mm tube to guide. The L-120×400 F is the smallest class that holds the die squarely at this diameter; a lighter frame deflects and the ovality shows up before the force limit does.
Talk to an engineer on WhatsApp
Send your tube drawing, material and target output. We will reply with a machine configuration, a measured sample plan and a factory quotation. WhatsApp +86 183 0020 2909 or email info@jixin.online.
Chat on WhatsApp