What ovality control means at 76 → 48 mm

Short version for Aluminium 6061-T6 at 76 → 48 mm: 1.4 per cent ovality at the tip, held by a full-length guide bushing and a 5 mm die land. It is worth knowing why before you accept it, because the same three inputs that produce this answer will produce a different one the moment the wall or the grade changes.

Ovality is measured as the difference between the largest and smallest diameter at the same section. Above about 1 % of OD, a tapered end stops fitting the thing it was made for.

Three sources, in order of likelihood

Incoming tube ovality comes first and is the cheapest to check: measure both ends at four clock positions before the tube goes on the machine. A tube that is already 0.5 mm out will not be rounded by the die, it will be tapered oval. Budget 1.35 USD per piece at this combination, of which 75 per cent is metal.

Die closure is second: if the ovality lines up with the die parting line, the die is not closing evenly or the guide is off-centre. Third is the absence of a mandrel on thin wall, where the section collapses inward rather than resisting. Springback adds 0.071 mm to the tip diameter, so the die is cut that much under nominal.

What actually holds 1 %

A guide bushing within one tube diameter of the die entrance, a mandrel on any D/t above 40, and a die that closes on a parallel land rather than a taper. Those three together hold 0.5–1 % of OD on production parts. 20,473 pieces per die set is the working number here; below 10,236 pieces a year the tooling never pays back.

Measuring ovality with a caliper on a curved surface is unreliable. Use a two-point micrometer at 90°, or a ring gauge for anything that has to fit. The 3.7 per cent scrap allowance is not padding — it is the pass count and the material talking.

The numbers for this combination

Tube outside diameter76 mm
Small-end diameter48 mm
Wall thickness3.5 mm
Cone length120 mm
Reduction on diameter36.8 per cent
Half angle / included angle6.65° / 13.3°
Yield strength used275 MPa
Forming force, single bite277 kN
Forming force, per bite at 3 passes109 kN
Passes3 passes
Processcold forming
Cycle time17.1 s
Output per 8 h shift1,381 pieces
Tip wall after forming4.54 mm (+30 per cent)
Springback on tip diameter0.071 mm
Ovality at the tip1.4 per cent
Blank length214 mm
Blank weight0.461 kg
Machine classL-120×400 F

Computed for this combination. Confirm the force and the tip wall on a sample before the die is cut.

The force figure is the one people misread. 277 kN is what a single bite taking the whole 36.8 per cent reduction would need; the press in the schedule only sees 109 kN because the reduction is split. Quoting the first number for a multi-pass job is how machines get bought one size too large.

Read the table before the prose if you are in a hurry. The table is the part you can defend in a meeting; the prose explains which entries are sensitive to the material certificate and which are not.

How Aluminium 6061-T6 behaves at 36.8 per cent reduction

Forms at a third of the tonnage of steel and springs back three times as much. T6 temper is already precipitation-hardened, so the cone can crack if the reduction is aggressive.

Aluminium 6061-T6 at this reduction behaves like a demanding material, and the schedule above is written for that. Push the reduction per pass and the failure mode is a longitudinal split starting at the tip edge, not a slow drift out of tolerance.

Typical use for this grade is handlebars, seatposts, tent poles, display frames. If your part sits outside that list, the numbers still apply but the corrosion and fatigue assumptions behind them do not.

Large section: 76 → 48 mm

At 76 mm the force starts to matter: the same wall needs roughly twice the tonnage of a 60 mm part, and the guide bushing has to control a heavier tube.

At 76 mm the guide bushing matters as much as the die. A 76 mm tube has enough length to lever against the die entry if the bushing clearance is loose, and the symptom is ovality at the tip that looks like a die problem and is not.

Floor space and power follow the class, not the part: a L-120×400 F needs the footprint in its own datasheet whether you run 76 mm or something smaller in it.

Cost per 1,000 pieces

Metal in the blank0.461 kg, 1.013 USD
Machine time17.1 s, 0.143 USD
Die cost, one set2,970 USD
Die life20,473 pieces
Scrap allowance3.7 per cent
Cost per piece1.35 USD
Cost per 1,0001,351 USD

Scrap is priced into 1.35 USD at 3.7 per cent. If your first article runs clean, the real cost is lower than this; if it does not, this number was optimistic and the difference shows up as a month of rework.

What to put on the drawing

Say what happens after forming: machined, welded, coated, or used as formed. The allowance, the stress relief and the surface spec all follow from that one line.

Add the as-formed wall at the tip as a reference dimension with a minimum. It is the dimension that decides whether the mating bore cleans up, and it is the one most often left off.

Send the drawing as a PDF with the dimensions readable at 100 per cent. Half the quotation delays we see come from a photo of a printout, not from a hard part.

Frequently asked questions

Does ovality affect the taper angle?

It affects the measured angle, because the angle is derived from diameters. A 2 % oval tip can read as 0.5° of angle error that is not actually there.

Can ovality be corrected after forming?

A light sizing pass in a ring die can bring 1.5 % back to 0.8 %. Beyond that the part is scrap, because sizing marks the surface.

Is ovality worse on welded tube?

Usually yes, near the seam. The weld zone has different flow stress, so it resists the die slightly differently from the base metal.

Is 6061-T6 suitable for a part that will be welded after forming?

It welds, but the formed tip is work-hardened and the weld pool will dilute that. For a structural weld, stress relieve at 175 °C first, or move the weld away from the cone.

Would a smaller machine do this job?

Not at 109 kN per bite with a 76 mm tube to guide. The L-120×400 F is the smallest class that holds the die squarely at this diameter; a lighter frame deflects and the ovality shows up before the force limit does.