What ovality control means at 60 → 38 mm

Short version for Stainless 304 (08Kh18N10) at 60 → 38 mm: 1.3 per cent ovality at the tip, held by a full-length guide bushing and a 4 mm die land. It is worth knowing why before you accept it, because the same three inputs that produce this answer will produce a different one the moment the wall or the grade changes.

Ovality is measured as the difference between the largest and smallest diameter at the same section. Above about 1 % of OD, a tapered end stops fitting the thing it was made for.

Three sources, in order of likelihood

Incoming tube ovality comes first and is the cheapest to check: measure both ends at four clock positions before the tube goes on the machine. A tube that is already 0.5 mm out will not be rounded by the die, it will be tapered oval. The mill certificate matters more than the grade name: spread inside the standard moves the force by about 7 kN.

Die closure is second: if the ovality lines up with the die parting line, the die is not closing evenly or the guide is off-centre. Third is the absence of a mandrel on thin wall, where the section collapses inward rather than resisting. At this size the die sees 68 kN per bite, which is why the L-120×400 F is the natural home for the job.

What actually holds 1 %

A guide bushing within one tube diameter of the die entrance, a mandrel on any D/t above 40, and a die that closes on a parallel land rather than a taper. Those three together hold 0.5–1 % of OD on production parts. Running 2 passes puts the cycle at 12.0 s and the shift output near 1,968 pieces.

Measuring ovality with a caliper on a curved surface is unreliable. Use a two-point micrometer at 90°, or a ring gauge for anything that has to fit. The tip wall finishes at 3.14 mm, 26 per cent heavier than the 2.5 mm you started with — plan the mating bore around that and not around the blank.

The numbers for this combination

Tube outside diameter60 mm
Small-end diameter38 mm
Wall thickness2.5 mm
Cone length95 mm
Reduction on diameter36.7 per cent
Half angle / included angle6.60° / 13.2°
Yield strength used215 MPa
Forming force, single bite122 kN
Forming force, per bite at 2 passes68 kN
Passes2 passes
Processcold forming
Cycle time12.0 s
Output per 8 h shift1,968 pieces
Tip wall after forming3.14 mm (+26 per cent)
Springback on tip diameter0.058 mm
Ovality at the tip1.3 per cent
Blank length171 mm
Blank weight0.612 kg
Machine classL-120×400 F

Computed for this combination. Confirm the force and the tip wall on a sample before the die is cut.

The force figure is the one people misread. 122 kN is what a single bite taking the whole 36.7 per cent reduction would need; the press in the schedule only sees 68 kN because the reduction is split. Quoting the first number for a multi-pass job is how machines get bought one size too large.

Read the table before the prose if you are in a hurry. The table is the part you can defend in a meeting; the prose explains which entries are sensitive to the material certificate and which are not.

How Stainless 304 (08Kh18N10) behaves at 36.7 per cent reduction

Low yield but severe work hardening: the cone gets hard as it forms, so the die load climbs through the stroke. Galling is the main risk and it is a lubrication problem before it is a die problem.

Stainless 304 (08Kh18N10) at this reduction behaves like a workable material, and the schedule above is written for that. Push the reduction per pass and the failure mode is a roughened cone that needs polishing, not a slow drift out of tolerance.

Typical use for this grade is food equipment, architectural tube, exhaust tips. If your part sits outside that list, the numbers still apply but the corrosion and fatigue assumptions behind them do not.

Medium section: 60 → 38 mm

The 60 to 38 pair is the workhorse of the trade: fork blanks, furniture legs, pole sections. Tonnage is moderate and almost every machine size can do it, so the decision usually turns on cycle time and die life.

At 60 mm the guide bushing matters as much as the die. A 60 mm tube has enough length to lever against the die entry if the bushing clearance is loose, and the symptom is ovality at the tip that looks like a die problem and is not.

Floor space and power follow the class, not the part: a L-120×400 F needs the footprint in its own datasheet whether you run 60 mm or something smaller in it.

Cost per 1,000 pieces

Metal in the blank0.612 kg, 1.960 USD
Machine time12.0 s, 0.080 USD
Die cost, one set2,170 USD
Die life28,004 pieces
Scrap allowance2.2 per cent
Cost per piece2.16 USD
Cost per 1,0002,165 USD

Scrap is priced into 2.16 USD at 2.2 per cent. If your first article runs clean, the real cost is lower than this; if it does not, this number was optimistic and the difference shows up as a month of rework.

What to put on the drawing

Say what happens after forming: machined, welded, coated, or used as formed. The allowance, the stress relief and the surface spec all follow from that one line.

Add the as-formed wall at the tip as a reference dimension with a minimum. It is the dimension that decides whether the mating bore cleans up, and it is the one most often left off.

Send the drawing as a PDF with the dimensions readable at 100 per cent. Half the quotation delays we see come from a photo of a printout, not from a hard part.

Frequently asked questions

Does ovality affect the taper angle?

It affects the measured angle, because the angle is derived from diameters. A 2 % oval tip can read as 0.5° of angle error that is not actually there.

Can ovality be corrected after forming?

A light sizing pass in a ring die can bring 1.5 % back to 0.8 %. Beyond that the part is scrap, because sizing marks the surface.

Is ovality worse on welded tube?

Usually yes, near the seam. The weld zone has different flow stress, so it resists the die slightly differently from the base metal.

Is 304 stainless suitable for a part that will be welded after forming?

It welds, but the formed tip is work-hardened and the weld pool will dilute that. For a structural weld, stress relieve at 400 °C first, or move the weld away from the cone.

Would a smaller machine do this job?

Not at 68 kN per bite with a 60 mm tube to guide. The L-120×400 F is the smallest class that holds the die squarely at this diameter; a lighter frame deflects and the ovality shows up before the force limit does.

Talk to an engineer on WhatsApp

Send your tube drawing, material and target output. We will reply with a machine configuration, a measured sample plan and a factory quotation. WhatsApp +86 183 0020 2909 or email info@jixin.online.

Chat on WhatsApp