Defects at the tip

Crack at the tip: a split along the cone, usually starting at the small end. Cause is excessive reduction in one pass or a die entry radius that is too sharp. Check the reduction ratio first, then the die.

Folded tip: the wall has collapsed inward. Cause is thin wall with too fast a stroke, or a die cavity that is too long for the material to fill. Slow the stroke and check die length.

Thin tip wall: wall below drawing. Cause is a die that is oversized at the tip, or excessive springback not compensated in the die. Measure the die, not the machine.

Defects on the flank

Wrinkles: circumferential folds on the cone flank. Cause is a die angle that is too steep for the wall, or insufficient back pressure. Reduce the angle or add a pre-form pass.

Orange peel: a rough, matte surface. Cause is coarse grain in the parent tube or too fast a stroke. Change tube specification or slow down.

Die marks: longitudinal scoring. Cause is die surface finish, lubrication failure, or galling on stainless. Polish the die and change lubricant before touching force.

Step at the blend: a visible ridge where the cone meets the tube. Cause is a die whose entry diameter does not match the actual tube OD, often because the tube is at the top of its mill tolerance.

Defects that are not the die's fault

Eccentric cone: TIR out of tolerance. Cause is die-to-tube misalignment, tube bow, or uneven clamp. Check alignment with a test bar before adjusting anything else.

Length drift: taper start point moving part to part. Cause is blank length variation or a feed that is slipping. Measure ten blanks before blaming the die.

Frequently asked questions

Which defect is most common?

Die marks and orange peel on cosmetic parts, cracks at the tip on thick wall. Both are solved by die finish and stroke speed.

Can a cracked tip be reworked?

No. A crack at the tip is a scrap part; welding it changes the material and the geometry. Cut it off and re-form if length allows.

How do I tell a die problem from a machine problem?

Run ten parts and measure the die. If the cone matches the die, the machine or the blank is at fault; if it does not, the die is.

Talk to an engineer on WhatsApp

Send your tube drawing, material and target output. We will reply with a machine configuration, a measured sample plan and a factory quotation. WhatsApp +86 183 0020 2909 or email info@jixin.online.

Chat on WhatsApp