What a 40 → 25 mm taper asks of the die
This geometry removes 37.5 per cent from the outside diameter over a 120 mm cone. The included cone angle is 7.2°, and at a 1.0 mm starting wall the material has to flow inward rather than be cut away.
Force is driven by the 205 MPa yield, the 1.0 mm wall and the 37.5 per cent reduction. One bite means 31 kN; with 2 passes the die sees around 17 kN.
Tip wall and springback on this part
Constant volume puts the wall at the small end near 1.26 mm, 26 per cent heavier than the 1.0 mm blank. If the mating bore was dimensioned from the starting wall, it will not assemble. Add the as-formed tip wall to the drawing as a reference dimension with a minimum.
Measure the cold part: recovery on this grade is about 0.032 mm on diameter and ovality near 2.0 per cent. Ring-gauge at a fixed distance from the end every time.
How 316L stainless behaves at 40 mm outside diameter
Softer than 304 at the start and just as eager to work-harden. Molybdenum makes it galling-prone in a different way: it welds to the die rather than scratching it.
Changeover time decides the minimum batch size that is worth running. Below that number, the honest answer is to quote higher or decline.
At 205 MPa yield with medium ductility, this grade needs 2 passes on this geometry. The die is expected to last 17,387 pieces before the first re-polish, and the stress-relief practice is: Anneal after heavy deformation; low carbon means no sensitisation risk at the weld.
Typical applications are chemical plant, marine hardware, medical frames. If your part sits outside that list, the forming numbers still apply but the corrosion and fatigue assumptions may not.
Cycle, tooling and piece cost
Cycle time is about 11.4 seconds from tube in to tube out, which is roughly 2,071 pieces in an eight-hour shift at 82 per cent utilisation. The die is expected to make 17,387 pieces before the first re-polish.
At the current price band the formed part costs about 0.95 USD, of which roughly 66 per cent is the blank. The recommended class is the Ø50 class (manual or automatic); a larger frame buys stiffness this diameter does not use.
How to quote this geometry
A readable drawing with OD, tip, cone length, wall and grade is enough for a first quote. Add the downstream operation so the allowance and the stress relief are specified rather than assumed.
For Stainless 316L (03Kh17N14M2) the decision that moves the number most is changeover economics. Say what you need there before asking for a price.
Frequently asked questions
What machine class forms a 40 → 25 mm tube?
The Ø50 class (manual or automatic). Forming force is about 17 kN per bite with 2 passes, so a smaller frame will deflect before it stalls.
How much thicker is the tip?
From 1.0 mm to about 1.26 mm, an increase of 26 per cent. Machine the bore after forming if the fit is tight.
What should I put on the drawing?
The two diameters, cone length, wall, grade and the as-formed tip wall. Add springback compensation of about 0.032 mm on the die.